Our existing demolding article explains why draft matters and what happens when there is not enough of it. This article is the reference piece: the actual numbers to use for each plastic, each surface finish, and each draw condition.
If you are drafting a part for injection moulding and want to know what minimum angle to assign to a specific wall, this is the chart to use.
Why one number does not work
The common rule — "use one degree of draft per side" — is a floor, not an answer. The real draft requirement varies by:
- Material shrinkage — higher shrinkage releases more easily; lower shrinkage grips the core
- Surface finish — a polished surface releases freely; a textured surface mechanically keys to the steel
- Draw depth — deeper draws need more draft to release in the same vertical travel
- Wall orientation — walls parallel to the draw direction (external walls) release differently from internal walls over a core
- Material modulus — stiff, filled materials are less forgiving than flexible unfilled ones
Baseline draft angles by material
Values below are minimum draft per side for polished (SPI A-2 or better) surfaces on moderate draw depths (under 50 mm). Deeper draws and textured surfaces need more; see the sections below for adjustments.
| Material | Minimum draft (polished) | Notes |
|---|---|---|
| Polyethylene (PE, HDPE, LDPE) | 0.25° to 0.5° | High shrinkage, flexible — releases easily |
| Polypropylene (PP) | 0.5° to 1.0° | Standard baseline |
| Polystyrene (PS, HIPS) | 0.5° to 1.0° | Low ductility, needs clean release |
| ABS | 0.5° to 1.0° | Standard baseline |
| Polycarbonate (PC) | 1.0° to 2.0° | Low shrinkage, grips core |
| PC/ABS blend | 1.0° to 1.5° | Between PC and ABS values |
| Polyamide (PA6, PA66) unfilled | 0.5° to 1.0° | Standard baseline |
| Polyamide (PA6-GF30, PA66-GF30) | 1.0° to 1.5° | Lower shrinkage with glass fill |
| Polyacetal (POM, Delrin) | 0.5° to 1.0° | Good release, high shrinkage |
| PBT, PET | 0.5° to 1.0° | Standard baseline |
| PMMA (acrylic) | 1.0° to 2.0° | Low shrinkage, scratch-sensitive |
| TPE, TPU (soft) | 2.0° or more | High friction, soft release |
| Rigid PVC | 1.0° to 2.0° | Low shrinkage, prone to sticking |
| LCP | 0.5° to 1.0° | Low shrinkage anisotropic — simulate flow direction |
Material datasheets from MatWeb and Omnexus give shrinkage ranges that correlate with draft requirements; higher-shrinkage grades at the top of the range need less draft than lower-shrinkage grades.
Draft adjustments for surface finish
Textured surfaces are the single biggest multiplier on draft requirement. The texture is cut into the mould steel, and the plastic flows into it, keying mechanically. To release, the part has to slide out of every one of those micro-undercuts.
Industry rule from the SPI (now PLASTICS) and widely adopted VDI texture standards:
| Finish | Add to baseline draft | Description |
|---|---|---|
| SPI A-1 (optical) | 0° | Diamond polish, no addition |
| SPI A-2, A-3 | 0° | Fine polish, baseline values apply |
| SPI B-1, B-2, B-3 | +0.5° | Stone/paper finish |
| SPI C-1, C-2, C-3 | +1.0° | Stone finish, visible marks |
| VDI 3400 ref 18-24 (light grain) | +1.0° to +1.5° | Common fine texture |
| VDI 3400 ref 27-33 (medium grain) | +2.0° to +3.0° | Common medium texture |
| VDI 3400 ref 36-42 (coarse grain) | +3.0° to +5.0° | Common heavy texture |
| Mold-Tech MT-11010 (medium) | +2.0° to +3.0° | Reference texture, confirm with supplier |
| Leather and heavy grains | +5.0° or more | Validate with texture supplier (Mold-Tech, Standex) |
Texture suppliers such as Mold-Tech by Standex publish specific draft recommendations for each of their patterns. When specifying a textured finish, pull the supplier's datasheet for the exact pattern and depth — generic rules miss by a lot on deep textures.
Deep draw calculation
For walls deeper than 50 mm, the required draft to release the part in a reasonable ejector stroke increases. Use this geometric calculation:
Minimum release gap = Draw depth × tan(draft angle)
Rearranged for the draft angle given a target release gap:
Draft angle (degrees) = atan(release gap / draw depth)
A reasonable target release gap at the end of ejector stroke is 0.5 mm minimum on polished surfaces, more on textured. For a 100 mm deep wall with a 0.5 mm release target:
Draft = atan(0.5 / 100) = 0.29° — which is why deep draws often need 1° to 2° just for geometric release, before any material or texture factor.
Draft on ribs and bosses
Ribs and bosses have their own draft rules because they are usually core-pulled rather than cavity-pulled, and because they are thinner than the main wall. From our rib and boss design guide:
- Ribs: 0.5° to 1° per side on each flank, with rib root at 60% of nominal wall
- Bosses (external): 0.5° on the outside wall, nominal wall thickness
- Bosses (internal, cored): 0.25° to 0.5° on the core, often less because the shrinkage grip is on the core itself
Draft on undercut areas
If a feature cannot be released on the main parting line, it needs a side action or lifter. Draft on side-action faces is measured relative to the direction of the slide travel, not the main draw direction. Standard practice:
- 0.5° to 1° on side action faces, polished
- +1° to +2° on textured side-action faces
- 0° on the sealing face between slide and cavity (otherwise flash forms)
Zero-draft walls — when and how
Occasionally a design calls for a wall with no draft at all (bosses for threaded inserts, sealing surfaces, snap-fit catching faces). Zero draft is possible but needs:
- Highly polished surface (SPI A-1 or A-2)
- Short feature height (under 5 mm typically)
- Material with high shrinkage (PA, POM, PE) that pulls away from the steel
- Mould release spray or coating on the steel, used sparingly
- Confirmation during tool trials — expect to add draft if ejection is marginal
Zero-draft walls are the exception, not a feature to design into every surface. Each zero-draft spot adds trial-and-error cost at the tool tryout stage.
When draft can be reduced
Three design or process choices allow draft below the baseline values:
- Polished SPI A-1 surface — reduce baseline by 0.25° if the part is not deep
- Highly flexible material (TPE, soft PE) with low modulus — baseline may be excessive
- Core-pulled features that are short and shallow — the slide handles the release, draft is secondary
Common mistakes to avoid
From our experience reviewing DFMs and tool trials:
- Specifying 0° draft on cosmetic walls because "it looks better in CAD"
- Applying one global draft value to a part with mixed polished and textured surfaces
- Forgetting that ribs need their own draft, not inherited from the main wall
- Specifying a VDI texture without checking the texture supplier's minimum draft
- Measuring draft from the parting line without accounting for the actual draw direction after side actions
For related design mistakes that drive up tooling cost, see our top 10 design mistakes article.
Validation during tool design
Draft should be verified in CAD before the tool is cut. Any good CAD system (Siemens NX, PTC Creo, SolidWorks, CATIA) has a draft analysis function that colour-codes faces by angle relative to the pull direction. Running this analysis is a 10-minute check that saves tool rework.
For complex geometries, a mould flow and ejection simulation in Moldflow or Moldex3D can predict ejection force. If predicted force exceeds the ejector system capability, draft needs to increase or the ejection system needs to be reconsidered.
How FD Group handles draft on new programmes
Every DFM review we do includes a draft analysis using the part's intended material and finish specification. If the design cannot accommodate the required draft without changing the aesthetic intent, we flag the trade-off before the tool is cut, not after. If you want a DFM review on an upcoming part, get in touch and we will walk through the draft and release implications of your design.